Pitting corrosion attributes & folklore

Written on: March 1, 2025 by W. Stephen Tait

Hello, everyone. Metal pitting corrosion causes product and propellant leakage from spray packages. Pitting corrosion typically happens very fast; it could occur almost anywhere inside a spray package and significantly reduces a package’s service lifetime.

This column will review both the attributes of pitting corrosion and the five most common instances of folklore concerning spray package pitting corrosion.

Pitting corrosion attributes
The four main attributes of metal pitting corrosion are:

1. Pitting occurs in small, discrete, localized areas on both coated and uncoated metal surfaces (coating blisters are also localized corrosion)

2. Pitting corrosion has three stages: 1] initiation (also called nucleation); 2] growth to a critical size; and 3] growth until the metal perforates and leaks

3. Pits need a support area surrounding them to sustain their high rate of corrosion (hence the localized areas are discrete and small)

4. The chemical composition of an environment (a formula) and the type of package materials (e.g., uncoated/coated metals and metal foils) determine both if pitting corrosion occurs and the rate of pitting corrosion

The rate of pitting corrosion determines the package service lifetime.

Folklore 1: Pits begin at holes in the tin coating on tinplated steel containers
Tinplated steel (ETP) is a steel sheet sandwiched between two very thin coatings of metallic tin. Tin coatings are typically specified by the total weight of tin on both sides per sheet surface area. Tin coatings can also be thicker inside containers, referred to as “differential ETP.”

The tin coating on ETP is not a perfect coating. Indeed, approximately 20% of the tin coating for 0.25-pound ETP is a combination of exposed iron-tin alloy and exposed steel.

Holes in tinplate might, or might not, cause galvanic corrosion between the tin and the steel. The chemical composition of a formula determines if galvanic corrosion will occur, the steel or the tin will corrode in your formula, and how fast the galvanic pitting will perforate the steel.

Holes in tin coatings are not deep enough to initiate and sustain galvanic pitting corrosion; therefore, metal exposure through holes is not needed to cause ETP container pitting corrosion. For example, I’ve seen numerous instances where pitting began after the edge of complete detinning (tin corrosion) was far enough from the center of the detinned area to cause pitting around the center of the completely detinned area.

Folklore 2: Pits begin at holes in a polymer coating

Folklore 3: A hole in polymer coating concentrates corrosion, thereby causing pitting
These two examples of folklore are discussed together because they involve polymer coated aluminum or steel and both are actually the result of pitting attribute #3: A pit needs a support area surrounding it to sustain a high pitting corrosion rate.

Holes are common in polymer coatings. However, polymer coating holes are also not deep enough to initiate metal substrate pitting without additional factors. A large amount of area around each pit is needed for the water, the electrochemical active ions and molecules in a formula to diffuse through the coating and react with the electrons generated by metal corrosion inside the pit. In other words, a large amount of the coated area must fail (corrode) to initiate and sustain pitting under a coating.

Folklore 4: No pitting corrosion after three months of storage testing at a high temperature is a good acceptance criterion
I’ve observed numerous instances with storage stability tests where:

1. Packages stored at high temperatures had pitting corrosion that was not present in the corresponding packages stored at room temperature

2. Pitting corrosion occurred in packages stored at room temperature, but not the corresponding packages stored at higher temperatures

3. There was no difference in the pitting corrosion rates for the packages stored at room temperature and the corresponding packages stored at high temperatures

These observations support the conclusion that temperature does not accelerate package pitting corrosion.

In addition, daily ambient temperatures are cyclic, seasonal and variable. Consequently, three months of continuous storage testing at ≥ 90° F (≥ 32° C) rarely correlates with actual years of variable seasonal temperatures where spray products are purchased and used.

Recent global climate research also indicates that local climate patterns are changing. For example, the wildfire season caused by Santa Ana winds in California has shifted from October/November to December/January. Consequently, traditional high temperature storage parameters, such as test length and temperature, are probably no longer valid.

Folklore 5: Pitting corrosion is caused by defects in the metal
This corrosion folklore is partially true. Pitting corrosion could begin at microscopic crystal and metallurgical defects (see the March, April and May 2024 editions of Corrosion Corner for examples of crystal and metallurgical defects). However, these defects are an inherent property of all metal alloys, and there are multiple-millions of these defects per surface area on the aluminum, the tin-free steel and the ETP metals used to fabricate spray packaging.

In other words, defects do not cause pitting by themselves. Metal pitting corrosion is caused by the interaction of a formula chemistry with metal defects that determines if, where and how fast pitting corrosion penetrates a package’s metal or metal foil.

Pitting corrosion can be detected with both long-term storage stability tests (one year minimum needed) and electrochemical corrosion tests (a significantly shorter time needed). rustdr@pairodocspro.com. SPRAY