Worst-case corrosion testing?

Written on: October 1, 2025 by W. Stephen Tait

In this age of faster-to-market timetables, there are often pressures on formulators and engineers to accelerate the various tests needed to qualify new products and derivatives for existing products (line extensions). These pressures often tempt one to use worst-case testing to obtain quicker results. The reasoning is often that a product that passes worst-case testing will be OK under normal conditions.

However, worst-case testing often provides misleading results. For example, would you conduct a consumer test with a group who never uses one of your products and who never intend to use it (worst-case group)? The thought process would be, “If this group likes it, everyone will like it.” Of course you wouldn’t, as results from such a group would probably provide extremely misleading future sales estimates for a product.

The same is true for container corrosion testing. A firm would not want to use results from test conditions that don’t reflect actual use by the majority of its consumers. Some examples of worst-case testing for aerosol container corrosion include testing at high temperatures—and using the results to estimate lifetime at room temperature—and testing containers in an inverted position.

Figure 1 illustrates how worst-case testing could provide container corrosion results that are significantly different from the corrosion found during typical consumer use. The Y-axis in Figure 1 is the cumulative percent container failures (e.g., perforations, doesn’t spray, etc.) for a population of containers (e.g., one year of production). The X-axis is the number of days prior to container failure. For example, the:

 

• Left graph has 15% failures after 400 days of worst-case testing
• Right graph has no failures after 400 days and only 0.1% failures after 860 days (2.4 years)

 

The two graphs in Figure 1 illustrate how a failure profile developed from worst-case corrosion test data could be significantly different from the actual use failure profile. Indeed, worst-case failure profiles could lead to rejecting a commercially viable product.

Inverting aerosol containers in a storage test is often viewed as a worst-case situation for the aerosol valves and valve gaskets. However, the corrosion mechanism for materials submerged in liquids is very different from the mechanism for materials in vapors. Indeed, there are ample papers available in corrosion literature that shows corrosion of materials submerged in liquids is significantly more severe than corrosion of materials in vapors.

For most situations, I recommend avoiding worst-case testing for aerosol container corrosion testing. However, in some instances there may be an unusual consumer-use-practice that is different from the normal-use-practices for your products. For example, you might have a product where aerosol containers are stored and used in the inverted position. Testing this group of products with the aerosol containers inverted would not be worst-case testing for this situation. However, inverting containers to accelerate vapor phase corrosion and evaluate valve gasket corrosion would be worst-case (and incorrect) corrosion tests.

Thanks for your interest and I’ll see you in November. Contact me at 608-831-2076; rustdr@pairodocspro.com or from our two websites: pairodocspro.com and aristartec.com. SPRAY